FABRICATION:-
Lower work hardening rate makes bending and forming somewhat easier than for grade 304
Lower ductility restricts very severe operations.
Severe bends should be made with the bend axis at right angles to the rolling direction.
Severe cold heading of 430 wire is possible.

| C | Mn | P | S | Si | Cr | Fe |
| 0.12 Max. | 1.00 Max. | 0.040 Max. | 0.030 Max. | 1.00 Max. | 16.0 – 18.0 | Balance |

Heat Treatment
Solution annealing can be performed by heating stainless steel grade 430 to 815 - 845°C (1499-1553°F). Then it has to be slow furnace cooled to 600°C (1112°F) and followed by air-cooling in a quick manner - as slow cooling between 540 and 400°C (1004 and 752°F) tends to cause embrittlement.
For sub-critical annealing, heating should be performed to 760-815°C (1400-1499°F), followed by air-cooling or water quenching.
This stainless steel cannot be hardened by thermal treatment.